@@ -26,9 +26,12 @@
"p_b(T)": "Vapor pressure \(p\) in pascals: \[\log(p/Pa) = 5.006 + A + BT^{-1} + C\log{T} + DT^3\] where temperature T in K; p. 6-72",
"Electromagnetic Data": {
"chi_m": "Magnetic susceptibility; Molar susceptibility \[\chi\ti{m} = \kappa V\ti{m} = \kappa M / \rho \] where \(\kappa\) is the volume susceptibility, \(V\ti{m}\) is the molar volume of the substance, \(M\) the molar mass, and \(\rho\) the mass density. \(\kappa = \bold{M}/\bold{H}\) where \(\bold{H}\) is the magnetic filed and \(\bold{M}\) is magnetic moment per unit volume.",
"Electrical conductivity": ""
},
"Mechanical Properties": {
"T": "Reference temperature",
"Temperature": "Reference temperature",
"Density": "Density",
"Young modulus": "Module of elasticity",
"Yield strength": "R_{p0.2}",
"Ultimate tensile strength": "R_m",
"Elongation": "A_5",
@@ -38,11 +41,12 @@
},
"Thermodynamic Properties": {
"Crystal, Liquid, Gas": {
"Delta_f H°": "Standard molar enthalpy (heat) of formation at 298.15 K in kj/mol. 0.0 indicates the reference state.",
"Coefficient of thermal expansion": "",
"Delta_f H°": "Standard molar enthalpy (heat) of formation at 298.15 K in kJ/mol. 0.0 indicates the reference state.",
"Delta_f G°": "Standard molar Gibbs energy of formation at 298.15 K in kJ/mol",
"S°": "Standard molar entropy at 298.15 K in J/mol K",
"S°": "Standard molar entropy at 298.15 K in J/mol/K",
"cp": "Specific heat capacity",
"Cp": "Molar heat capacity at constant pressure at 298.15 K in J/mol K",
"Cp": "Molar heat capacity at constant pressure at 298.15 K in J/mol/K",
},
"Delta_vap H": "Molar enthalpy (heat) of vaporization. Values are given at a pressure of 101.325 kPa",
"Delta_fus H": "Molar enthalpy (heat) of fusion. Values are given at the normal melting point Tm"
@@ -90,8 +94,14 @@
"color": "silvery-white metal",
"crystal": "cubic|cubic crystals"
},
"Electromagnetic Data": {
"chi_m": [16.5e-6, "cm³/mol"],
"Electrical conductivity": ["16-18", "m/Ω/mm²"]
},
"Mechanical Properties": {
"T": ["20-25", "°C"],
"Temperature": ["20-25", "°C"],
"Density": [2.66, "g/cm³"],
"Young modulus": [70, "GPa"],
"Yield strength": ["110-130", "MPa"],
"Ultimate tensile strength": ["230-290", "MPa"],
"Elongation": ["10-15", "%"],
@@ -99,6 +109,11 @@
"HBW": ["68-75", "2.5/62.5"]
}
},
"Thermodynamic Properties": {
"Crystal": {
"Coefficient of thermal expansion": [23.3, "m/µm/K"]
}
},
"Source": [
{
"Type": "Book",

View File

@@ -43,7 +43,7 @@
],
"rho(T)": {
"rho_m": [2.375, "g/cm³"],
"k": [0.000233, "g/cm³ °C"],
"k": [0.000233, "g/cm³/°C"],
"Tmax": [1340, "°C"]
},
"p_b(T)": {
@@ -69,16 +69,16 @@
"Crystal": {
"Delta_f H°": [0.0, "kJ/mol"],
"Delta_f G°": null,
"S°": [28.3, "J/mol K"],
"cp": [0.897, "J/g K"],
"Cp": [24.20, "J/mol K"]
"S°": [28.3, "J/mol/K"],
"cp": [0.897, "J/g/K"],
"Cp": [24.20, "J/mol/K"]
},
"Liquid": null,
"Gas": {
"Delta_f H°": [330.0, "kJ/mol"],
"Delta_f G°": [289.4, "kJ/mol"],
"S°": [164.6, "J/mol K"],
"Cp": [21.4, "J/mol K"]
"S°": [164.6, "J/mol/K"],
"Cp": [21.4, "J/mol/K"]
},
"Delta_vap H": [
[
@@ -162,8 +162,13 @@
"Heat treatment": {
"Temper": "homogenized and stress relieved, O3"
},
"Electromagnetic Data": {
"Electrical conductivity": ["16-18", "m/Ω/mm²"]
},
"Mechanical Properties": {
"T": ["20-25", "°C"],
"Temperature": ["20-25", "°C"],
"Density": [2.66, "g/cm³"],
"Young modulus": [70, "GPa"],
"Yield strength": ["110-130", "MPa"],
"Ultimate tensile strength": ["230-290", "MPa"],
"Elongation": ["10-15", "%"],
@@ -171,6 +176,11 @@
"HBW": ["68-75", "2.5/62.5"]
}
},
"Thermodynamic Properties": {
"Crystal": {
"Coefficient of thermal expansion": [23.3, "m/µm/K"]
}
},
"Source": {
"Type": "Web",
"URL": "https://gleich.de/en/wp-content/uploads/sites/4/2016/10/en_g.al_c250.pdf"